Le Prometheus® Metal Clay are a remarkable material: they work like clay, but after firing, they become true pure metal, such as bronze or copper!

They consist of:

  • micronised metal powders
  • water
  • organic binder

During firing, water and binder evaporate and burn away, leaving only the sintered metal, solid and durable. You can shape them by hand, roll them out, create coils, engrave, imprint textures, just like you would with regular modelling clay. And you can even combine them together and fire them alongside many synthetic gems!

Each of them has specific firing and finishing characteristics that we will discover in this useful guide.

Common characteristics

Each Prometheus® clay has different firing temperatures, but shaping, storage, and drying work the same way for all.

When you open the package, the so-called “wet phase” begins. In this phase, the clay is soft, ready to be shaped and very pleasant to work with. It does not tend to stick to either hands or plastic surfaces, but a useful little trick is to lightly oil your fingers and work surface with a drizzle of olive oil.

You can work it on a smooth plastic surface, on wax paper, or on a Teflex sheet. Simple tools are enough for shaping: your fingers, a rolling pin, a few spatulas, or a toothpick. Even everyday objects can become tools for creating interesting textures.

Shaping

It is important not to work it for too long. Over time, it tends to dry out and may start to crack. If you notice small cracks, don’t panic: just lightly moisten the surface with a brush and fill the cracks with a bit of cream made by mixing clay and water until you reach a consistency similar to thick yogurt.

While working, remember to always store scraps in the bag and seal the package well. If you do not plan to use it for a few days, you can place the bag in a sealed jar with a slightly damp sponge at the bottom: a small tip that helps keep it in ideal conditions. Periodically check the sponge and add water if necessary.

Drying before firing

Before firing, the piece must be completely dry. This step is essential because if moisture remains inside, the piece may crack or deform in the oven. You can let it dry naturally at room temperature, or speed up the process with a hairdryer or by placing it above a warm oven (not recommended for large pieces). Food dehydrators also work very well.

A simple method to check that it is truly dry is the “mirror test”: place the hot piece on a cold mirror. If no condensation appears, it is ready for firing.

Once dry, you can refine your work: file, sand, engrave, or drill. At this stage, the material is more fragile than the final metal, so it should be handled carefully, but it is also the ideal time to correct imperfections and make the surface more even.

The different firing methods

Firing is the phase that transforms the clay into metal. Before starting, it is always advisable to do a test with a small sample to check the accuracy of the oven.

Electric ovens may have slight temperature variations; based on the test result, you can adjust the firing temperature by ±5% until you achieve the correct sintering.


With Activated Carbon (recommended)

Step 1: place the dry piece on a grid made of stainless steel, insert it into the cold oven, and bring to 500 °C for 15 minutes. Let cool.

Step 2: put about 3 cm of activated carbon at the bottom of a steel container, position the pieces spaced at least 1.5 cm apart, and cover them completely with carbon. Insert the container into the preheated oven at 820 °C and fire for 60 minutes. Let cool in the oven.

With Oven Grid

Place the pieces on a grid made of stainless steel in the preheated oven at 820 °C, taking utmost care with the high temperatures. Since the temperature will tend to drop upon opening, close the door again and wait for the oven to return to the set value and fire for 30 minutes. At the end, let the pieces cool inside the oven until the temperature has significantly lowered. When the heat has dropped to a safer level, extract using appropriate high-temperature resistant tools and immerse in warm water with pickle to remove most of the oxidation. Be cautious of the vapours generated by wearing a mask.

With Torch

This type of application is very complex. Even experienced users tend to avoid it because it is easy to ruin the piece: oxidation occurs very quickly in the presence of air. For this reason, unless you have already experimented, we do not recommend this firing method.


With Activated Carbon (recommended)

Step 1: place the dry piece on a grid made of stainless steel, insert it into the cold oven, and bring to 500 °C for 15 minutes. Let cool.

Step 2: put about 3 cm of activated carbon at the bottom of a steel container. Position the pieces spaced (at least 1.5 cm apart) and cover them completely with carbon. Close the container and insert it into the preheated oven at 850 °C and fire for 90 minutes. Then let cool in the oven.

With Oven Grid

Place the pieces on a grid made of stainless steel in the preheated oven at 920 °C, taking utmost care with the high temperatures. Since the temperature will tend to drop upon opening, close the door again and wait for the oven to return to the set value and fire for 30 minutes. At the end, let the pieces cool inside the oven until the temperature has significantly lowered. When the heat has dropped to a safer level, extract using appropriate high-temperature resistant tools and immerse in warm water with pickle to remove most of the oxidation. Be cautious of the vapours generated by wearing a mask.

With Torch

This type of application is very complex. Even experienced users tend to avoid it because it is easy to ruin the piece: oxidation occurs very quickly in the presence of air. For this reason, unless you have already experimented, we do not recommend this firing method.


With Activated Carbon (recommended)

Step 1: place the dry piece on a grid made of stainless steel, insert it into the cold oven, and bring to 500 °C for 15 minutes. Let cool.

Step 2: put about 3 cm of activated carbon at the bottom of a steel container. Position the pieces spaced (at least 1.5 cm apart) and cover them completely with carbon. Close the container and insert it into the preheated oven at 820 °C and fire for 60 minutes. Then let cool in the oven.

With Oven Grid

Place the pieces on a grid made of stainless steel in the preheated oven at 820 °C, taking utmost care with the high temperatures. Since the temperature will tend to drop upon opening, close the door again and wait for the oven to return to the set value and fire for 30 minutes. At the end, let the pieces cool inside the oven until the temperature has significantly lowered. When the heat has dropped to a safer level, extract using appropriate high-temperature resistant tools and immerse in warm water with pickle to remove most of the oxidation. Be cautious of the vapours generated by wearing a mask.

With Torch

This type of application is very complex. Even experienced users tend to avoid it because it is easy to ruin the piece: oxidation occurs very quickly in the presence of air. For this reason, unless you have already experimented, we do not recommend this firing method.


With Activated Carbon

Step 1: place the dry piece on a grid made of stainless steel, insert it into the cold oven, and bring to 500 °C for 15 minutes. Let cool.

Step 2: put about 3 cm of activated carbon at the bottom of a steel container. Position the pieces spaced (at least 1.5 cm apart) and cover them completely with carbon. Close the container and insert it into the preheated oven at 770 °C and fire for 120 minutes. Then let cool in the oven.

For thin and elongated pieces, annealing is recommended to maintain high strength. To do this, place the pieces in a preheated oven at 565 °C, wait 5 minutes, then remove them and immerse them in water and pickle.

The final colour of both (PWB and PSW) is similar to silver. The PWB is more heat sensitive than the PSW.


With Activated Carbon

Step 1: place the dry piece on a grid made of stainless steel, insert it into the cold oven, and bring to 500 °C for 15 minutes. Let cool.

Step 2: put about 3 cm of activated carbon at the bottom of a steel container. Position the pieces spaced (at least 1.5 cm apart) and cover them completely with carbon. Close the container and insert it into the preheated oven at 780 °C and fire for 60 minutes. Then let cool in the oven.


With Activated Carbon

Step 1: place the dry piece on a grid made of stainless steel, insert it into the cold oven, and bring to 500 °C for 15 minutes. Let cool.

Step 2: put about 3 cm of activated carbon at the bottom of a steel container. Position the pieces spaced (at least 1.5 cm apart) and cover them completely with carbon. Close the container and insert it into the preheated oven at 800 °C and fire for 60 minutes. Then let cool in the oven.


How to combine different metal clays

It is possible to combine different Prometheus® Metal Clays in the same piece and fire them together using the two-phase method with carbon. The temperature of the second phase should be set according to the clay with the lowest sintering temperature, and the firing must be for at least 2 hours.

Also, consider the shrinkage rates of each of them, listed below:

  • PCC® 9–10%
  • PBC® 12–13%
  • PSB® 12–13%
  • PSW® 15–16%
  • PGY® 13–14%
  • PLY® 17–19%
  • PWB® 10–11%

Finishing (for all Prometheus clays)

After firing, the piece appears dull and oxidised. This is normal. This is when the magic of finishing begins. Start by brushing the surface with a metal brush, then rinse and dry.

You can then apply patinas to achieve different effects and colours.

Finally, proceed with polishing, using abrasive papers, polisher, or tumbler. Using abrasive pastes significantly increases the shine, bringing out all the beauty of the metal.

Safety and precautions

Prometheus® clays are non-toxic and do not contain harmful substances, but it is always good practice to work in a well-ventilated environment during firing. Use gloves, safety glasses and tongs to handle hot pieces and containers, and always place the material on heat-resistant surfaces.

No explicit or implied warranty is provided regarding the accuracy of the data in this guide. The user is responsible for verifying the suitability of the product and its safe use.


Article created in collaboration with Paola Mattioli